玻璃瓶"剪刀印”解析與解決方案 玻璃瓶"剪刀印”解析與解決方案 Analysis and solution of glass bottle "scissor printi Release time: 2020-06-09 Visited: 4659 Times

In the forming process of glass container, the drop forming is the first step of the bottle forming process, and it is also the key to the glass bottle forming process.


Drop forming is to make the drop glass liquid have a suitable and uniform temperature. Under the mechanical motion of the barrel, bowl, punch and scissors, the drop glass liquid forms to meet the requirements of forming.


The defect of glass containers (bottles and cans) "scissor print" is the obvious trace left on the bottles and cans due to poor shearing during the forming process of the material drop.


A kind of


1、 Shear process of droplet formation


The glass liquid flowing out of the bowl is cut by overlapping and closing the upper and lower scissor pieces to form the glass drop. In the process of shearing, the glass drops are impacted by the temperature of the scissors and the mechanical force of the scissors.


When the bad shear occurs, it is possible to produce glass shear marks on two parts of the material drop. The shear mark on the material drop will be left at the bottom of the glass bottle, and the shear mark under the material drop will be left at the mouth of the glass bottle. This kind of cutting trace will enlarge in the process of forming and blowing, forming a "scissors print".


"Scissor print" affects the appearance slightly, and becomes the source of crack.


A kind of


2、 The formation of scissor print


When the glass liquid flowing out of the bowl is cut off by the scissors, the glass liquid left in the upper part of the bowl mouth is suspended, and the glass liquid drop in the lower part falls into the mold through the guide material. When the suspension glass liquid and the lower glass drop which are cut off and left at the mouth of the bowl are cut, the scissors mark of the scissors will be left. Because of its large heat, the suspension glass liquid at the material bowl mouth can reduce the temperature difference through heavy heat and eliminate the scissor print generated by the upper scissor blade. However, because the lower glass droplet contacts with the mold and cools rapidly, it is easy to leave the scissor print generated by the lower scissor blade.


In the shear process of material drop formation, the glass liquid is cut through overlapping and closing of scissors. If:


1. If the sharpness of the scissors is not good, the cutting section of the glass liquid flowing out of the material bowl will be stuck, stretched or pushed in the horizontal direction of the upper and lower scissors. The glass liquid stretched or pushed by adhesion will cool faster than the whole material drop. In the conveying process of the material drop to the primary die through the guide chute, the glass liquid that is stuck, stretched or pushed by the heavy heat of the material drop during the shearing process may reach the same temperature as the whole material drop. It will not affect the whole material drop.


However, the effect of reheating is not good. The temperature of the glass liquid produced in the process of shearing may not be consistent with the temperature of the whole material drop, so the glass liquid produced in the process of shearing will form tiny bubbles in the material drop. The "scissor print" is formed during the molding and blowing process.


2. The amount of overlapping of the scissors is not enough, so that the scissors are not enough overlapped and closed, and the material drop is not completely cut when cutting the glass liquid. A glass drawing wire is formed between the hanging glass liquid and the shearing glass drops from the bowl mouth, which may cause tiny glass bulges at the upper and lower ends of the glass drops. The temperature of the glass bulge will drop rapidly, forming glass fragments attached to the surface of the glass drop, forming "scissors print" during the molding and blowing process.


A kind of


3. If the scissors are not tensioned enough, there will be a gap between the upper scissors and the lower scissors. When cutting the glass liquid, the cutting surface of the glass drops will be rough. If the roughness of the upper and lower cut surfaces cannot reach the same temperature with the whole material drop by reheating, a "scissor print" will be formed during the molding and blowing process.


A kind of


Under normal circumstances, the upper scissor blade is squeezed from the lower scissor blade, and the lower scissor blade is squeezed from the upper scissor blade. When the glass drops are cut off, the upper scissor and the lower scissor should be in a state of seamless overlap on the contact surface.


4. If the scissors are over tensioned, the squeezing pressure of the upper and lower scissors will become the resistance of each other's movement. This kind of resistance affects the amount of overlapping of the scissors, which makes the scissors not close enough and forms the glass drawing wire when cutting the glass liquid. In the process of forming and blowing, glass drawing will become "scissors printing".


5. The improper scissor cam makes the cutting action too slow. In the process of shearing, glass liquid is impacted by temperature and mechanical force of scissors. If the cutting action is too slow, more cutting marks will be left when cutting.


6. The cutting edge of the scissors should be sharp so that the glass liquid can be cut off easily. If the cutting edge of the scissors becomes blunt, the force of the blunt cutting edge on the surface of the liquid glass will increase when it is cut, and the cutting surface of the liquid glass will produce wrinkles. In the process of molding and blowing, the wrinkles on the cutting surface will become "scissors printing".


To ensure the sharpness of the scissors, the first is to timely replace the scissors; the second is to ensure good cooling in the production process.


7. Scissors spray too much or too little. In order to ensure the sharpness of the scissors, the temperature of the scissors must not be too high, so it is necessary to cool the cutting scissors, especially the cutting edge of the scissors.


Scissor water spray is the only way to cool scissor blade, but scissor water spray must be appropriate. Too small scissor water spray makes scissor blade not cool enough, and the blade of scissor blade becomes blunt, which will produce "scissor print". The scissors spray too much water, and the coolant is continuously sprayed on the glass liquid, causing the temperature of the glass liquid surface to drop, making the glass liquid shear badly, and also producing "scissors print".


The water spray of scissors can not only cool the scissors, but also lubricate the mutual movement of the upper and lower scissors

主站蜘蛛池模板: 日本一二三区视频在线| 日本乱子人伦在线视频| 人与禽性视频77777| 色久悠悠婷婷综合在线亚洲| 丰满岳乱妇bd在线观看中字| 乌克兰少妇videos高潮| 国产成人无码精品久久久小说 | 香蕉久久夜色精品国产| 国产成人午夜福利在线播放| 国产精品va在线播放我和闺蜜| 人妻换人妻aa视频| 欧美成人看片一区二区三区尤物| 日韩插啊免费视频在线观看| 日本十八禁视频无遮挡| 久久久久九九精品影院| 国产麻豆精品久久一二三| a级精品国产片在线观看| 隔壁邻居是巨爆乳寡妇| 婷婷射精av这里只有精品| 护士张开腿被奷日出白浆| 亚洲av综合a色av中文| 脱了我奶罩亲我奶头好舒服| 少妇人妻偷人精品一区二区| 久久人人爽人人爽人人片av高清 | 久久99久久99精品免观看| 少妇下面好紧好多水真爽播放| 最近2019中文字幕国语免费版| 亚洲色大成网站www久久九九| 手机看片福利一区二区三区| 邻居少妇张开双腿让我爽一夜| 大肉大捧一进一出视频| 亚洲国产精品尤物yw在线观看| 久久久久亚洲av无码永不| 国产18禁黄网站免费观看| 99国产欧美久久久精品| gogogo免费高清看中国国语| 亚洲欧美日韩高清一区| 免费a级毛片18禁网站免费| 久久亚洲av成人无码国产电影| 国产乱码一区二区三区爽爽爽| 在线 | 一区二区三区|